Gunite vs Shotcrete Pools in Southern Arizona
Gunite and shotcrete are the same sprayed concrete placed two ways: gunite is dry-mix, where dry cement and sand are blown through the hose and the nozzleman adds the water at the nozzle, and wet-mix shotcrete is concrete that is fully mixed, water included, before it is pumped to the nozzle. Either one can build a strong, watertight pool shell in Southern Arizona. The crew, the mix, the steel, the engineering and the curing decide the result far more than the name on the bid.
Around Tucson the word gunite gets used loosely for any sprayed concrete pool, so a bid or a neighbor that says gunite may mean either process. The American Concrete Institute has used the word shotcrete for both since at least 1967, and the American Shotcrete Association treats gunite as the dry-mix process only. If the process matters to you, ask which one the crew shoots and who is on the nozzle.
Gunite vs shotcrete at a glance
| Item | Dry-mix (gunite) | Wet-mix shotcrete | Source |
|---|---|---|---|
| What goes through the hose | Dry cement and sand, carried by air | Concrete fully mixed with its water, usually ready-mix, pumped | American Shotcrete Association Position Statement 2, using ACI 506 terms |
| Who controls the water | The nozzleman, at the nozzle | The batch plant, before the truck arrives | American Shotcrete Association Position Statement 2; PHTA Builder’s Manual, 5th ed., ch. 7 |
| Typical rebound on walls | 15 to 25 percent | 0 to 5 percent | PHTA Builder’s Manual, 5th ed., ch. 7 |
| Typical rebound on floors | 5 to 15 percent | 0 percent | PHTA Builder’s Manual, 5th ed., ch. 7 |
| Stopping and restarting | Dry material can be covered and restarted at will | A batched load has limited working time, and heat shortens it | PHTA Builder’s Manual, 5th ed., ch. 7 |
| Nozzleman certification | ACI Shotcrete Nozzleman, dry-mix process | ACI Shotcrete Nozzleman, wet-mix process | ACI Shotcrete Nozzleman certification policy |
| Fact that applies to both | Value | Source |
|---|---|---|
| Recommended minimum strength for pool shotcrete | 4,000 psi at 28 days | American Shotcrete Association Position Statement 1 |
| Concrete temperature when it leaves the truck | 95°F maximum unless testing or past field experience supports more | ACI 301-20 and ACI 305.1-14, per ACI’s published FAQ |
| What ACI counts as hot weather | Any combination of high air temperature, high concrete temperature, low humidity and high wind | ACI 305R-20, Guide to Hot Weather Concreting |
| Reinforcing steel before shooting | Shade or wet it to keep it under 100°F | PHTA Builder’s Manual, 5th ed., ch. 7 |
| Moist curing | Continuously moist at least 7 days, then wet at least once a day through day 28 | American Shotcrete Association Position Statement 7 |
| Concrete cover over steel against the ground | At least 3 inches | American Shotcrete Association Position Statement 8; AMMTEC standard detail plan |
| Pima County permit engineering baseline | #3 bar at 12 inches on center each way; floor #3 bar at 6 inches each way in highly expansive soils and wash areas | AMMTEC Consultants standard detail plan, Pima County master plan P18MP00069 D2, 2018-11-28 |
| Omni’s typical schedule | #3 bar at 6 by 12 inches, tightened to 6 by 6 on expansive or collapsible soil; most Catalina Foothills lots at 6 inches on center | Omni house standard; the sealed engineering for each pool governs |
| Nozzleman certification terms | Separate exam and test panel for each process; vertical position required; good for 5 years | ACI Shotcrete Nozzleman certification policy |
| National residential inground pool standard | ANSI/PHTA/ICC-5 2025, published June 3, 2025 | Pool and Hot Tub Alliance |
| Caliche | Soil cemented by calcium carbonate, in layers from a few inches to several feet thick | University of Arizona Cooperative Extension, AZ1281 |
| Expansive soil | Clay that swells when wet and shrinks as it dries, enough to crack slabs and foundations | Arizona Geological Survey, problem soils |
Last checked November 2026.
What the difference means on a pool
In the hands of a certified nozzleman, both processes produce dense, well-bonded concrete. The differences are in control and waste. With dry-mix, the nozzleman sets the water by eye at the nozzle, which takes skill and lets the crew start and stop at will. With wet-mix, the water is set at the batch plant, so each load leaves at a known mix, and far less material bounces off the walls.
Rebound is the material that bounces off. It carries less cement than the mix that stays in place, so it has to be cleaned out of the hole and off the steel rather than buried in the shell. Dry-mix throws more of it, so the cleanup matters more.
Strength comes from the mix either way. The American Shotcrete Association recommends at least 4,000 psi at 28 days for pool shotcrete. On dry-mix, strength follows the ratio of cement to sand, and the PHTA Builder’s Manual pairs a 1 to 4 mix with about 4,000 psi and leaner mixes with less. On wet-mix, the builder orders a design mix from the plant and the plant weighs every batch.
A pool shot in more than one session has a joint where new material meets old. The American Shotcrete Association’s position is that a properly prepared joint between shotcrete layers is a construction joint that stays monolithic, not a cold joint: taper the edge, clean off overspray, roughen it, dampen it and keep shooting. Joints come up more often in hot weather because material stiffens faster.
What Southern Arizona changes
Heat. ACI 305R-20 treats hot weather as a combination of high air temperature, high concrete temperature, low humidity and wind, and a Southern Arizona summer brings all four. ACI 301-20 and ACI 305.1-14 cap concrete at 95°F when it leaves the truck unless testing or past field experience supports more. The PHTA Builder’s Manual adds field rules: wet the subgrade before shooting, shade or wet the steel to keep it under 100°F, keep materials and hoses shaded at 85°F and above, and shoot early in the morning when the schedule allows. It also notes that wet-mix crews commonly add a retarder above 85°F.
Curing. In hot weather the American Shotcrete Association wants curing started as soon as the shell allows. It calls for keeping the shell continuously moist for at least 7 days, soaking it three to five times a day or more, then wetting it at least once a day through day 28, and more often in hot, dry places. Plastic sheeting holds moisture in on some jobs, but the PHTA Builder’s Manual says it is not an acceptable method in extremely hot climates.
Caliche and rock. University of Arizona Cooperative Extension describes caliche as soil cemented by calcium carbonate, in layers from a few inches to several feet thick and sometimes as hard as rock. Rock and caliche dig out with rough faces and voids, and shotcrete fills whatever the excavation leaves, so a rocky lot means more material, not a thinner shell. Shotcrete also has to pass behind every bar. On our jobs a void behind the steel is exposed and repaired, never patched over. Most Catalina Foothills lots we build on get rebar at 6 inches on center and extra shotcrete to fill the rock voids, and the sealed engineering for each lot sets the final spacing.
Expansive soil. The Arizona Geological Survey describes clays that swell when wet and shrink as they dry, enough to crack slabs and foundations. The permit engineering accounts for it. The AMMTEC standard detail plan used on many Pima County permits doubles floor steel to #3 bar at 6 inches each way in highly expansive soils and in wash areas, and calls for the shell to bear on firm undisturbed native soil or on engineered fill compacted to at least 95 percent of maximum density under ASTM D698.
The engineer sets the shell, not the builder. Arizona has no codified minimum for pool shell reinforcement, so the sealed engineering in the permit set governs bar size, spacing, cover and shell thickness. The AMMTEC sheet maps soil category and pool depth to shell thickness and bar counts. The PHTA Builder’s Manual says a licensed engineer should provide the rebar size and spacing for each pool, and the American Shotcrete Association leaves splices, cover and extra layers of steel to the licensed design professional. ANSI/PHTA/ICC-5 2025, the national standard for residential inground pools, covers their design and installation, but the numbers on your shell come from the engineering for your lot. A builder can build heavier than the sheet, never lighter.
Which process Omni uses
Omni’s shells are wet-mix shotcrete: ready-mixed concrete delivered by truck and pumped to the nozzle, shot over steel set to the engineer’s schedule. Our typical minimum is #3 bar at 6 by 12 inches, tightened to 6 by 6 on expansive or collapsible soil. Most people in Tucson call that a gunite pool.
What to ask a builder about the shell
- Which process the crew shoots, dry-mix or wet-mix, and whether the shotcrete crew is the builder’s own or a subcontractor.
- Whether the nozzleman holds an ACI Shotcrete Nozzleman certification for that process. A dry-mix certification does not cover wet-mix.
- What strength the mix is designed for. The industry recommendation for pools is at least 4,000 psi at 28 days.
- What soil category your engineering sheet assumes, and what bar spacing and shell thickness it calls for at your depth.
- How rebound and overspray will be cleaned out, and how a joint will be prepared if the shell is shot in more than one session.
- What the curing plan is for the first 7 days and through day 28, and who does the watering.
- When you can see the steel and plumbing before they are covered.
Common questions
Is gunite the same as shotcrete?
Gunite is one kind of shotcrete. It is the old trade name for dry-mix, where the water is added at the nozzle. Shotcrete covers both dry-mix and wet-mix, and around Tucson people say gunite for either one.
Is wet-mix or dry-mix better for a pool?
Neither is better in every case. Both build strong, watertight shells when a certified nozzleman shoots a proper mix over engineered steel and the shell is cured. Wet-mix arrives at a batched mix and throws less rebound. Dry-mix lets the crew stop and restart at will and depends more on the nozzleman’s water control.
Does Tucson heat hurt a new shotcrete pool?
It can if the crew ignores it. ACI’s specifications limit concrete to 95°F when it leaves the truck unless testing or field experience supports more, and the PHTA Builder’s Manual calls for keeping the steel under 100°F, wetting the subgrade and shooting early in the day. The bigger risk is the shell drying out in its first week, which is a curing problem.
How long does a new pool shell need to be watered?
The American Shotcrete Association calls for keeping the shell continuously moist for at least 7 days, then wetting it at least once a day through day 28. In hot, dry weather that means soaking it three to five times a day or more for the first week.
Who decides how thick the shell is and how much steel goes in?
The engineer. Arizona has no codified minimum for pool shell reinforcement, so the sealed engineering in your permit set governs. On many Pima County permits that is the AMMTEC standard detail plan, which sets #3 bar at 12 inches on center each way as the baseline and #3 at 6 inches each way in the floor for highly expansive soils and wash areas. Omni’s typical minimum is #3 bar at 6 by 12 inches, tightened to 6 by 6 on expansive or collapsible soil.
Does caliche or rock change how the shell is built?
It changes the hole, not the design. Rock and caliche dig out with rough faces and voids, and shotcrete fills them, so a rocky lot takes more material, not a thinner shell. Most Catalina Foothills lots we build on also get rebar at 6 inches on center, and the sealed engineering for each lot sets the final spacing.
What is a cold joint, and should I worry about one?
A cold joint forms when new concrete is placed against material that has set too far to bond with it. The American Shotcrete Association’s position is that a joint between shotcrete layers stays monolithic when the edge is tapered, cleaned, roughened and dampened before shooting resumes. Ask how the crew prepares a joint, especially in summer, when they happen more often.
What should I ask to see from the nozzleman?
Ask for the ACI Shotcrete Nozzleman certification and check that it covers the process being used, dry-mix or wet-mix. ACI certifies each process separately with its own exam and test panel, requires the vertical shooting position, and the certification is good for 5 years.
Sources
- https://shotcrete.org/faq-items/what-is-the-difference-between-shotcrete-and-gunite/
- https://shotcrete.org/wp-content/uploads/2022/02/Definitions-of-Key-Shotcrete.pdf
- https://shotcrete.org/wp-content/uploads/2020/01/ASAPositionPaper_PoolRec_1.pdf
- https://shotcrete.org/wp-content/uploads/2022/02/Monolithic-Shotcrete_Position-Statement.pdf
- https://shotcrete.org/wp-content/uploads/2022/01/218216_SCMSummer21_PS7v2.pdf
- https://shotcrete.org/wp-content/uploads/2025/06/Pool-position-statement-steel-reinforcement-for-shotcreted-pools-1.pdf
- https://www.concrete.org/frequentlyaskedquestions.aspx?faqid=15
- https://www.concrete.org/Portals/0/Files/PDF/Previews/305R-20_preview.pdf
- https://www.concrete.org/Portals/0/Files/PDF/scn.pdf
- https://www.phta.org/media-center/newsfeed/phta-icc-publish-phta-5-2025-inground-residential-pool-standard
- https://www.extension.arizona.edu/publication/managing-caliche-home-yard
- https://azgs.arizona.edu/center-natural-hazards/problem-soils
- PHTA Builder’s Manual, 5th edition, Chapter 7 (shotcrete placement, rebound, hot weather and curing)
- AMMTEC Consultants, PLLC, Standard Gunite and Reinforcement Detail Plan, Pima County approved master plan P18MP00069 D2, 2018-11-28
Related reading
- What the engineered reinforcement sheet in a Pima County pool permit requires
- Omni’s typical reinforcing schedule and what to compare it against
- What your builder should show you before the plumbing and steel are covered
- The hold points in a pool build
- Who is responsible for knowing the soil under a new pool
- Custom pool building in Tucson
- Pool remodeling and resurfacing in Tucson